Bronze C95300

Annealing Procedure

The annealing temperature for this alloy is between 1150 and 1225 F or 620 and 660 C. The time at temperature is one hour per inch of section thickness.

Heat Treatability

The stress relieving temperature of this alloy is 600 F or 316 C. The time at temperature is one hour per inch of section thickness. This alloy does respond to heat treatment. The solution heat treating temperature is between 1585 and 1635 F or 860 and 890 C. The time at temperature is one hour per inch of section thickness. The quenching medium is water.

Machinability

The machinability rating of this alloy is 55. (Where Alloy 360 FC Brass is 100).

Principle Design Features

Cast - Bronzes (Copper-Aluminum-Iron and Copper-Aluminum-Iron-Nickel)

Weldability

Soldering of this alloy is rated as "good", brazing is rated as "good", oxyacetylene welding is "not recommended", carbon arc welding is rated as "fair", gas shielded arc welding is rated as "excellent", and coated metal arc welding is rated as "good".

Known Forms

Coil

Coil

Disc

Disc

Flat Bar

Flat Bar

Foil

Foil

Hexagon Bar

Hexagon Bar

Hollow Bar

Hollow Bar

Pipe

Pipe

Plate

Plate

Ring

Ring

Rod

Rod

Round Bar

Round Bar

Round Tube

Round Tube

Sheet

Sheet

Square Bar

Square Bar

Strip

Strip

Additional Data

Specifications

B148,B30,B505,B763,B806,C-11866,C390,J461,J462,C95300

Chemical Elements

Aluminum9 - 11
Copper86 nom
Iron0.8 - 1.5
Remainder TotalCu + sum of named elements 99.0 min

Physical Properties

Density: 0.323lb/in³Density