Nickel Vanadium Permendur (tm)

Annealing Procedure

This is a 49% Ni/ Co alloy with 2% vanadium. It possesses excellent magnetic and physical properties including high saturation flux density, low DC coercive force and high permeability at high inductions.

Applications

This alloy is used in motor laminations, transducers, poles and cores as well as transformer and head laminations.

Cold Workability

This material has a very high work hardening rate.

Formability

Due to its high cobalt content, this alloy can be quite difficult to form.

Heat Treatability

For optimum properties, it is essential that proper post work annealing be performed. Heat to 1540 F for 2 hours in pure hydrogen and cool slowly at a rate of 180 to 200 F per hour. Temperatures above 1600 F will cause damage to the material's potential properties.

Machinability

Generally not produced in machinable forms.

Principle Design Features

Soft magnetic alloy, 49% Fe-, 9% Co, 2% V. Very easily cracked in forging.

Known Forms

Coil

Coil

Disc

Disc

Flat Bar

Flat Bar

Foil

Foil

Hollow Bar

Hollow Bar

Pipe

Pipe

Plate

Plate

Rectangle Tube

Rectangle Tube

Ring

Ring

Rod

Rod

Round Bar

Round Bar

Round Tube

Round Tube

Sheet

Sheet

Square Bar

Square Bar

Strip

Strip

Additional Data

Specifications

A801 Alloy Type 1

Chemical Elements

Cobalt49 nom
Iron49 nom
Vanadium2 nom

Physical Properties

Density: 0.292lb/in³Density

Mechanical Properties

Thermal Expansion: 9.8µin/in·°FThermal Expansion

Mechanical Test Data

FormStrip
ConditionAnnealed
Temperature70°F
Brinell Hardness35 HB
Elongation1%
Tensile Strength175 KSI
Yield Strength185 KSI