Stainless
Stainless Sanicro 28 tm)
Applications
Applications include tubulars for downhole deep corrosive wells, pollution control, radiation waste systems, chemical handling equipment, valves pumps and piping.
Machinability
Conventional machining techniques used for iron based alloys may be used. Machining characteristics are somewhat similar to those for the austenitic (300 Series) stainless steels. This alloy does work-harden during machining and has higher strength and "gumminess" not typical of steels. Heavy duty machining equipment and tooling should be used to minimize chatter or work-hardening of the alloy ahead of the cutting. Most any commercial coolant may be used in the machining operations. Water-base coolants are preferred for high speed operations such as turning, grinding, or milling. Heavy-duty lubricants work best for drilling, tapping, broaching or boring. Rigid mounting of tooling and the workpiece are important to avoid "chatter".
Principle Design Features
This is a "super austenitic" stainless designed for resistance to phosphoric and sulfuric acids and seawater.
Known Forms
Angle
Channel
Coil
Disc
Flat Bar
Foil
Hexagon Bar
Hollow Bar
Pipe
Plate
Precision Ground Bar
Rectangle Tube
Ring
Rod
Round Bar
Round Tube
Sheet
Square Bar
Square Tube
Standard Beam
Strip
Tee
Additional Data
Specifications
B668,B709,1.4563,N08028Chemical Elements
| Carbon | 0.02 nom |
| Chromium | 27 nom |
| Copper | 1 nom |
| Iron | Balance |
| Manganese | 2 nom |
| Molybdenum | 3.5 nom |
| Nickel | 31 nom |
| Phosphorus | 0.025 nom |
| Silicon | 1 nom |
| Sulphur | 0.015 nom |
Physical Properties
Density: 0.29lb/in³
Specific Heat: 0.11BTU/lb·°F
Mechanical Properties
Modulus of Elasticity – Tension: 28MSI
Thermal Conductivity
| Condition | Temperature | Conductivity |
|---|---|---|
| Annealed | 70 °F | 7.8 BTU/hr·ft·°F |
Thermal Expansion
| Condition | Min | Max | Expansion Coefficient |
|---|---|---|---|
| Annealed | 70 °F | 200 °F | 8 μin/in·°F |
| Annealed | 70 °F | 400 °F | 8.4 μin/in·°F |
| Annealed | 70 °F | 800 °F | 9.6 μin/in·°F |
Mechanical Test Data
| Form | Sheet |
| Condition | Annealed |
| Temperature | 70°F |
| Elongation | 35% |
| Tensile Strength | 80 KSI |
| Yield Strength | 30 KSI |